Kufotokozera:
E71T-8-H8 ndi electrode yodziteteza yokha, yachitsulo cha kaboni, yokhala ndi ma flux cored cored. Yapangidwira kuwotcherera popanda mpweya woteteza wa kaboni ndi zitsulo zina zotsika kwambiri komwe kumafunika kulimba kwabwino kwambiri kutentha kochepa. Slag yoziziritsa mwachangu imathandiza kuwotcherera m'malo onse. Ili ndi kusamutsa kosalala kwa globular, mawonekedwe abwino kwambiri a bead komanso slag yochotsedwa mosavuta. E71T-8-H8 yapangidwa kuti igwiritsidwe ntchito popanga zomangamanga monga kupanga mlatho, kumanga sitima ndi bwato, komanso kupanga zina zambiri.
Kugawa ndi Kuvomereza:
E71T-8-H8 pa AWS A5.20, ASME SFA 5.20
E71T8-A2-CS3-H8 pa AWS A5.36, ASME SFA 5.36
AWS D1.8 Chivomerezi, CWB E491T-8-H8, ABS 3YSA, DNV IIIYMS
Ubwino:
Imagwira ntchito pa polarity yolunjika (DCEN) popanda mpweya woteteza wakunja.
Kuzizira mofulumira kwa slag kumathandiza kwambiri kusungunula zinthu m'malo onse.
Imawonetsa kusamutsa kosalala kwa globular, kufalikira kochepa komanso matope ochotsedwa mosavuta.
Katundu Wamba wa Makina:
Mphamvu Yolimba Kwambiri (psi) 87,000
Mphamvu Yotulutsa (psi) 64,000
Kutalikitsa kwa Peresenti 27
Kapangidwe ka Ndalama Zomwe Zili M'gulu la Ndalama (wt%):
CMnSi P S Al
0.210.720.20 0.010 0.005 0.55
Magawo Othandizira Kuwetsa (DCEN):
| M'mimba mwake | WFS | AMPERAGE | VOTEJI | CTWD (IN.) |
| 1/16″ | 120 | 165 | 17-18 | 5/8 |
| 170 | 200 | 18-19 | 3/4 | |
| 220 | 235 | 20-21 | 1 | |
| 270 | 270 | 21-22 | 1 | |
| 350 | 310 | 23-24 | 1 | |
| .072″ | 125 | 185 | 18-19 | 3/4 |
| 175 | 220 | 20-21 | 1 | |
| 200 | 245 | 21-23 | 1 | |
| 225 | 265 | 22-24 | 1 | |
| 250 | 275 | 22-24 | 1 | |
| 5/64″ | 60 | 140 | 17-18 | 3/4 |
| 100 | 210 | 18-19 | 3/4 | |
| 150 | 255 | 21-22 | 1 | |
| 200 | 300 | 22-23 | 1 | |
| 250 | 330 | 23-24 | 1 |
*Ma parameter awa angagwiritsidwe ntchito m'malo onse. Kuthekera kogwiritsa ntchito chitsulo chosungunuka pamlingo wapamwamba wamagetsi kudzadalira makulidwe a mbale ndi luso la wowotcherera.
Wenzhou Tianyu Electronic Co., Ltd. idakhazikitsidwa mu 2000. Takhala tikugwira ntchito yopanga ma electrode owotcherera,ndodo zowotcherera, ndi zogwiritsidwa ntchito zowotcherera kwa zaka zoposa 20.
Zogulitsa zathu zazikulu zikuphatikizapo ma electrode olumikizira zitsulo zosapanga dzimbiri, ma electrode olumikizira zitsulo za kaboni, ma electrode olumikizira zitsulo zosapanga dzimbiri, ma electrode olumikizira zitsulo zopindika, ma electrode olumikizira zitsulo zopindika, ma electrode olumikizira zitsulo zopindika ndi nickel & cobalt, mawaya olumikizira zitsulo zosapanga dzimbiri & low alloy, mawaya olumikizira zitsulo zosapanga dzimbiri, mawaya olumikizidwa ndi mpweya, mawaya olumikizira zitsulo zopindika, mawaya olumikizira zitsulo zopindika, mawaya olumikizira zitsulo zopindika ndi nickel & cobalt ... ndi mkuwa, mawaya olumikizira zitsulo zopindika ndi TIG & MIG, ma electrode a tungsten, ma electrode olumikizira zitsulo zopindika ndi kaboni, ndi zina zowonjezera ndi zogwiritsidwa ntchito.