AWS E6013 (J421X) Electrode Yowotcherera ya Chitsulo cha Kaboni Yogwiritsidwa Ntchito Powotcherera Molunjika

Kufotokozera Kwachidule:

J421X (AWS E6013) ndi electrode yokhala ndi titaniyamu yambiri yokhala ndi potaziyamu yogwiritsidwa ntchito powotcherera zitsulo za kaboni.


Tsatanetsatane wa Zamalonda

Ma tag a Zamalonda

Kuwotcherera kwa Chitsulo cha KaboniElekitirodi

J421X                                                      

GB/T E4313

AWS A5.1 E6013

Kufotokozera: J421X ndi electrode yokhala ndi titaniyamu yambiri yophimbidwa ndi potaziyamu yogwiritsidwa ntchito powotcherera zitsulo za kaboni. Imatha kugwira ntchito molunjika, ndipo ndi yoyenera kuwotcherera pamalo onse okhala ndi magwiridwe antchito abwino kwambiri, ndipo ingagwiritsidwe ntchito pa AC ndi DC. Chowotchereracho ndi chosalala komanso choyera. Chozunguliracho ndi chokhazikika komanso chosavuta kubwerezanso, slag imatha kuchotsedwa mosavuta.

 Kugwiritsa Ntchito: Imagwiranso ntchito pa kulumikiza zitsulo za kaboni ndi mbale yachitsulo yolumikizidwa, makamaka, imagwiritsa ntchito kulumikiza mbale yopyapyala pamalo oyima komanso pansi popanda kulumikiza.

 

Kapangidwe ka mankhwala a chitsulo chosungunula (%):

C

Mn

Si

S

P

≈0.08

≈0.5

≈0.25

≤0.035

≤0.040

 

Kapangidwe ka makina a chitsulo chosungunula:

Chinthu choyesera

Kulimba kwamakokedwe

Mpa

Mphamvu yobereka

Mpa

Kutalikitsa

%

Mtengo wa zotsatira (J)

Kutentha Kwabwinobwino.

0℃

Chotsimikizika

≥420

≥330

≥17

—

—

Yayesedwa

460 ~ 540

370 ~ 420

≈25

≈80

≈70

 Kuyang'anira X-ray: Giredi II

 

Mphamvu yovomerezeka:

M'mimba mwake wa ndodo

(mm)

2.0

2.5

3.2

4.0

5.0

kuwotcherera panopa

(A)

50 ~ 70

60 ~ 100

80 ~ 150

160 ~ 200

180 ~ 250

 

Wenzhou Tianyu Electronic Co., Ltd. idakhazikitsidwa mu 2000. Takhala tikugwira ntchito yopangaelekitirodi yowotchereras, ndodo zolumikizira, ndi zinthu zolumikizira kwa zaka zoposa 20.

Zogulitsa zathu zazikulu ndi chitsulo chosapanga dzimbirielekitirodi yowotchereras, ma electrode olumikizira zitsulo za kaboni, ma electrode olumikizira zitsulo za low alloy, ma electrode olumikizira zitsulo za surfacing, ma electrode olumikizira zitsulo za nickel & cobalt alloy, mawaya olumikizira zitsulo zopepuka & low alloy, mawaya olumikizira zitsulo zosapanga dzimbiri, mawaya olumikizidwa ndi mpweya, mawaya olumikizira aluminiyamu, mawaya olumikizira zitsulo za arc. mawaya, mawaya olumikizira zitsulo za nickel & cobalt alloy, mawaya olumikizira zitsulo zamkuwa, mawaya olumikizira zitsulo za TIG & MIG, ma electrode a tungsten, ma electrode olumikizira zitsulo za kaboni, ndi zina zowonjezera ndi zogwiritsidwa ntchito.

 